Line problems in coating, potting and printing: possible causes

These are symptoms plants see in coating, potting and printing. A symptom can have several causes at once. They sit in the material, in how it is applied, in the curing equipment and in the board itself. For each symptom this page lists the possible causes the supplier documents name, with the source for each. We work out with you which of them apply on your line.

Talk it through with us

Coating and UV curing

  • UV coating still tacky after the tunnel

    Material

    • It can be normal: PT 4600 is dual-cure, slightly tacky right after UV, and moisture finishes it in 2–3 days.ELANTAS mail, 2024-06-21

    Curing

    • The dose is too low for the belt speed. In Hoenle’s lab, PT 4600 cured at 2 m/min; at 4 m/min (about 2,236 mJ/cm² UVA, scaled from the 2 m/min measurement) it stayed tacky and blue.Hoenle AG lab test, PT 4600, 2024
    • Less light reaches the part than the datasheet figure: lamp values are stated at a condition (for example “distance 0 mm”), and without focus the intensity drops quickly with distance.Hoenle AG flyer, Spot 40 IC; Hoenle AG training, 2025
    • The lamp gives less than it used to: reflectors and quartz filters wear, and burnt-on contamination reduces the light output.Hoenle AG website, process monitoring; Hoenle AG bluepoint LED manual
    • The spectrum: an LED lamp emits no UVC, so on materials that need UVC for the surface, it can stay soft while the depth cures.Hoenle AG training, 2025

    Substrate and handling

    • The coating was pre-cured before the lamp by daylight or UV inspection lamps, and then never reaches its full properties.PT 4600 TDS

    What we check on your line

    The dose measured at the part, and with which meter (every instrument reads a bit differently); film thickness against the TDS; the age of the lamp.

    Talk it through with usCalculate the dose

  • Coating still wet beside tall components

    Material

    • A UV-only cure where the board needs a dual-cure grade: PT 4600 post-cures by moisture in 2–3 days; PL 5621 D needs 90 °C for 30 min where resin runs under parts.PT 4600 TDS; PL 5621 D TDS

    Application

    • Applied by needle, jetting or swirl, the material flows under components, where the lamp has no line of sight.PL 5621 D TDS

    Curing

    • UV does not reach the shaded areas beside and under tall parts.PL 5621 D TDS; PL 5622-250 TDS
    • Lamp position: close to an LED array the intensity is high but uneven; spot optics cover a set area at their focus distance (about 7 mm at 10 mm).Hoenle AG training, 2025

    What we check on your line

    The lamp angle and the number of heads around tall parts; whether an oven step follows the lamp; the humidity in the hall for the moisture post-cure.

    Talk it through with usUV curing

  • Bubbles in the coating after washing the boards

    Application

    • ELANTAS’s failure pictures show pin holes from air bubbles or fisheyes, without one stated cause.ELANTAS conformal-coating training, 2025

    Curing

    • On solvent-borne grades, an oven that heats up too fast can cause bubbles; the TDS says to limit the ramp.PL 4122 E TDS; BZ 1807 M TDS

    Substrate and handling

    • “Residual water from washing the PCB can cause bubbles.”PT 4600 TDS; PL 5621 D TDS
    • The flux and the cleaning: the TDS recommends low-solids flux or alcohol-based cleaning.PL 5621 D TDS

    What we check on your line

    Drying time and temperature after washing; air whipped in at the valve or spray (pressure, nozzle); the flash-off time before the oven.

    Talk it through with usBectron® coatings

  • Bubbles and unreliable cure on a moisture-cure coating

    Material

    • Moisture picked up after transfer to another cartridge or applicator raises the viscosity; the TDS says to apply from the original cartridge and to use transferred material quickly.PT 4834 TDS

    Substrate and handling

    • “Any residual moisture or alcohol under the [...] PT 4834 will cause bubbles and unreliable curing.”PT 4834 TDS

    What we check on your line

    The flash-off time after the alcohol clean; how long material sits in the feed lines; whether cartridges are sealed between shifts.

    Talk it through with us

  • Bubbles when heat-curing AP 8100

    Material

    • A frozen cartridge or a broken seal: air and water start the cure inside the cartridge.AP 8100 TDS
    • Layer thickness: 1 mm cures at room temperature in about 1 hour, up to 3 mm takes 6 to 10 hours; a thick layer in a fast oven is at risk.AP 8100 TDS

    Curing

    • “Rapid heating may cause bubbles to form”; the TDS sets 60 °C as the maximum.AP 8100 TDS

    What we check on your line

    The oven ramp at the part, not the set point; the cartridge temperature before use (20 to 30 °C per the TDS).

    Talk it through with usBectron® coatings

  • Poor wetting or adhesion of the coating

    Material

    • ELANTAS’s failure pictures show insufficient levelling from incompatibility with the substrate, and dewetting at solder joints.ELANTAS conformal-coating training, 2025

    Substrate and handling

    • The coating is not compatible with the solder resist, paste or flux on the board.PL 1104 TDS; PL 1102 TDS
    • Flux residue or a wet surface.PK 4340 TDS

    What we check on your line

    Surface energy and cleanliness of the board after reflow; the time between cleaning and coating; viscosity at the valve or tank against the spec (solvent evaporation thickens a dip tank, PL 1104 TDS).

    Talk it through with us

  • Coating still tacky after the oven

    Material

    • The material is past its shelf life.ELANTAS, technical reply to a customer case, 2024
    • A large can opened often or decanted picks up contamination; ELANTAS proposed smaller packs in that case.ELANTAS, technical reply to a customer case, 2024
    • PK grades react slowly at 80 °C since a raw-material change; ELANTAS recommends 90 °C for all PK grades.ELANTAS customer information, PK range, April 2024

    Curing

    • The part may not reach the cure temperature for the full cure time. ELANTAS first asks whether the oven is calibrated and whether the material “really sees” the temperature for that time (PL 5622-250: 30 min at 90 °C).ELANTAS, technical reply to a customer case, 2024
    • A heat-curing material given no heat: PK 4340 left at room temperature was still not hard after 72 hours.ELANTAS, technical reply to a customer case, 2022

    What we check on your line

    A temperature logger on the part through the oven; the time since the can was opened; the oven zone profile.

    Talk it through with us

  • “The colour says it is cured. Is it?”

    Curing

    • On PT grades the change from blue to green/yellow shows UV cure, but it also depends on the lamp, film thickness and humidity, and it reverses over time.PT 4600 TDS; ELANTAS mail, 2024-06-21
    • In Hoenle’s lab, under-dosed samples stayed blue and tacky.Hoenle AG lab test, PT 4600, 2024
    • Dose meters differ from each other; compare readings from the same instrument only.Hoenle AG training, 2025

    What we check on your line

    The dose with a fixed sensor position (a moved or tilted sensor changes the reading); tack and adhesion, not colour.

    Talk it through with us

Several of these can apply at once. Send us the coating, the lamp and the belt speed, and we go through it with you.

Talk it through with us

Potting

  • Bubbles and out-gassing in cured potting

    Material

    • The mix ratio is off: “Excess hardener may lead to bubbles in the cured resin and possible out-gassing after curing.”PU 4501 TDS; PU 4533 TDS
    • Resin or hardener has absorbed moisture, and the mix expands or foams.PU 4526 TDS

    Application

    • Air stirred in while mixing; the TDS suggests a vacuum step before casting, or for some silicones a short rest (about 5 minutes).PU 4526 TDS; SG 75L2-30 TDS; SK 76V2-75 TDS

    Curing

    • Temperature swings during cure: for PU 4526 the TDS says to avoid changes above 10 °C per hour.PU 4526 TDS

    What we check on your line

    The ratio the meter-mix machine actually delivers (weigh a shot of each component); static mixer length and condition; whether the pump or pail feed draws air; whether the part was pre-dried; the batch size against the TDS test mass (larger quantities shorten the pot life and raise the exotherm peak, PU 4526 TDS).

    Talk it through with usBectron® potting

  • Air bubbles in clear polyurethane

    Material

    • Moisture: for a room-temperature cure the TDS says moisture must be excluded.PU 4501 TDS; PU 4533 TDS

    Application

    • Agitation or transfer whips air into the unfilled resin.PU 4501 TDS; PU 4526 TDS
    • Hand mixing traps air; the TDS points to meter-mix equipment or a vacuum step.PU 4522 TDS; PU 4526 TDS

    What we check on your line

    Dispense speed and needle depth (filling from the bottom); vacuum level and time (the TDS gives no value); the casting depth.

    Talk it through with us

  • Hardener reacts slowly, or arrived crystallised

    Material

    • An opened PH 4912, PH 4901 or PH 4913 container has aged in air; moisture reduces the reactivity.PU 4522 TDS; PU 4501 TDS
    • Crystallisation in cold transport: PH 4912 and PH 4901 below 0 °C, PH 4913 below 5 °C.PU 4522 TDS; PU 4537 / PH 4913 TDS
    • Some viscosity rise in storage is normal; the cured properties do not change.PU 4526 TDS

    Substrate and handling

    • To recover crystallised hardener, warm the whole drum to 70 °C (PU 4526: 70–80 °C), with no local overheating.PU 4526 TDS; PU 4522 TDS

    What we check on your line

    How the hardener tank on the machine is protected from air; the date the container was opened; the delivery temperature.

    Talk it through with us

  • Silicone hardens inside the dispenser after weeks

    Material

    • A warm line speeds this up: “A 10 °C increase in temperature will approximately halve the curing time.”SK 75V2-45 TDS

    Application

    • Cross-contamination between the A and B paths.SK 75V1-35 TDS

    What we check on your line

    The static mixer and valve flush routine; seals and dead zones in the valve; the cleaner used (not stated in the TDS).

    Talk it through with us

  • Potting too viscous at room temperature

    Material

    • Viscosity depends on temperature: PU 4526 mixed is 3,000–4,000 mPa·s at 25 °C and 1,600–2,000 mPa·s at 40 °C. Warming also shortens the pot life (12–22 min at 25 °C, 10–18 min at 40 °C).PU 4526 TDS N°2121 Rev. 4 (12/2024)
    • The filler settles, so properties vary from pail to pail unless it is stirred or rotated.PU 4522 TDS; PU 4526 TDS

    Application

    • On one-component PK grades the needle sets the shear: its diameter, length and the applied pressure substantially reduce the viscosity.PK 4340 TDS
    Initial mixture viscosity
    3,000–4,000 mPa·s
    Pot life (doubled initial viscosity)
    12–22 min
    Gel time, 100 ml at 25 °C
    40–60 min

    Source: ELANTAS TDS PU 4526 / PH 4912, N°2121 Rev. 4 (12/2024). The fill is schematic.

    What we check on your line

    Pail or drum temperature conditioning; whether the pump suits the viscosity; needle diameter and length.

    Talk it through with us

Several of these can apply at once. Send us the resin and hardener, the mix ratio and the cure schedule, and we go through it with you.

Talk it through with us

Printed electronics (VFP inks)

  • Printed silver track resistance above the calculation

    Material

    • The ink stayed on the screen past its screen life (30 to more than 60 minutes, per grade) and thickened.VFP technical data sheets LV-SELEC, SECTR-I01, SE
    • Stretchable SES: resistance varies with the degree of elongation after thermoforming.VFP technical data sheet SES

    Application

    • The deposit is thinner than the mesh in the TDS gives.VFP technical data sheet SE

    Curing

    • The cure is below the TDS time or temperature.VFP technical data sheet SE

    Substrate and handling

    • “Resistance depends on the real substrate, the real dryer profile and the real deposit thickness on your press.”VFP website, RFID/NFC antennas article; VFP technical data sheet SE

    Length 6 cm · Width 1 mm · Thickness 8 µm

    The track VFP’s SE datasheet bases its resistivity on: 6 cm × 1 mm × 8 µm.

    Calculate the track resistance

    What we check on your line

    Whether the oven time is dwell at temperature or time in the oven (not stated in the TDS); dry thickness; squeegee and off-contact settings.

    Talk it through with us

  • Carbon track resistance too high

    Material

    • The ink was diluted; dilution “would deteriorate the conductive properties”.VFP technical data sheets CEL001, CEL003
    • The wrong silver/carbon pair: CEL001 goes over SE, SETF or FSE; CEL003 over SELEC or LV-SELEC.VFP technical data sheets CEL001, CEL003

    Application

    • The wrong cleaning solvent on the press: SECTR-I01, for example, precipitates unless cleaned with SOLVCP-S01.VFP technical data sheet SECTR-I01

    What we check on your line

    The thinning log on the press; the screen time used; the cure.

    Talk it through with us

  • Ink does not stick to the plastic film

    Curing

    • Under-cure (see the silver track and dielectric rows).VFP technical data sheets SE, ECV003

    Substrate and handling

    • The film’s surface tension; film lots differ according to their origin.VFP website, labels market page; VFP technical data sheet SE
    • The corona treatment is not “recent and regular”.VFP website, labels market page
    • The substrate is not on the ink’s list (the ECV dielectrics, for example, are not listed for PI, glass, PVC or TPU).VFP technical data sheet ECV003

    What we check on your line

    A cross-cut test per EN ISO 2409, target class 0; film cleaning and anti-static; PET pre-shrink (not stated in the TDS).

    Talk it through with us

  • VFP dielectric under-cured under an LED lamp

    Material

    • Thickness: the breakdown value is stated for 2 layers, 30 µm.VFP technical data sheet ECV003

    Curing

    • ECV003 and ECV004 cure under a broad-spectrum mercury or xenon lamp at more than 300 mJ/cm²; VFP states no LED cure for them.VFP technical data sheet ECV003
    • The dose is below the specification. Higher doses than recommended are tolerated.VFP technical data sheet ECV003
    • Oxygen at the surface can inhibit the polymerisation in printing.Hoenle AG printing brochure

    What we check on your line

    The dose at the sheet with a meter; whether each ECV layer is cured separately (not stated in the TDS); the lamp’s age.

    We offer the VFP inks and Hoenle AG UV equipment together.

    Talk it through with usPrinted electronics

Several of these can apply at once. Send us the ink, the substrate and the drying or curing step, and we go through it with you.

Talk it through with us

A different symptom on your line? Write to us.

Ask for a sample, a TDS, a quote or a dose calculation

Tell us what you need. We reply within 24 hours, in Romanian or English.

What do you need?

The button opens your email program with the inquiry filled in; you send it from there. We use these details only to answer this inquiry. Privacy notice

Contact directly

Alexandru Nichifor
Sales & technical support

+40 771 709 622

nichiforlx@nalteksolutions.com

Naltek Solutions S.R.L.
Sat Comori, Com. Gurghiu, nr. 81, jud. Mureș 547298