UV curing: Hoenle AG LED systems matched to the coating’s dose

A UV-curing coating states the UVA dose it needs. The lamp, its working distance and the belt speed decide whether your line delivers it: dose = irradiance × time. Bectron® PT 4600, for example, asks for 2,500–3,500 mJ/cm² UVA. We offer Hoenle AG UV curing systems in Romania, calculate the dose for your line and, on request, measure it on site.

Hoenle AG application lab: an LED-UV unit over a lab conveyor
Hoenle AG application lab: an LED-UV unit over a lab conveyor. Image: Hoenle AG

Why UV: the cure takes seconds

Bectron® PT 4600 cures in 3 to 7 s under the lamp, at 2,500–3,500 mJ/cm² UVA; shadow areas then cure by moisture in 2 to 3 days. The heat-cured thick film PK 4340 needs 30 min at 90 °C in an oven. The solvent-borne PL 4122 E grades cure in 16 h at 23 °C. With a UV coating, the cure step on the line is a lamp over the belt.

UV
PT 4600 · 3 to 7 s
Oven
PK 4340 · 30 min at 90 °C
Air
PL 4122 E · 16 h at 23 °C

LED or broadband lamp: what the coating needs

The coating’s photoinitiator decides whether it cures under LED (365–405 nm) or needs a broadband lamp. LEDs cure well in depth; broadband lamps also emit UVC, which helps the surface cure. An LED line therefore starts with a trial on your own part. ELANTAS developed PT 4600 for broad UVA curing; LED can work as well, and we confirm it for your line in a trial.

A printed film in a UV curing conveyor with a broadband lamp
A printed film passes through a UV curing conveyor with a broadband lamp, in a laboratory under yellow safety light. Image: ELANTAS Europe

Which Hoenle AG unit reaches the dose: intensity, wavelength, belt speed

Read the dose in the coating’s TDS, in mJ/cm². Read the unit’s intensity in mW/cm² at the wavelength the coating cures at. Window length and belt speed give the time under the lamp, and intensity × time gives the dose. The Hoenle AG page works this through for PT 4600 under an LED Powerline ACIC 820 XP. The UV dose calculator runs it for your lamp and line.

Two Hoenle AG LED Powerline ACIC heads, lit, over a moving belt
Two Hoenle AG LED Powerline ACIC heads, lit, over a moving belt. Image: Hoenle AG

A calculation gives the dose on paper. On the line we measure it at the part with a UV meter, as a service we quote per inquiry. Compare readings from the same instrument only: dose meters differ from each other.

UV dose calculator · How to calculate UV dose on a conveyor

Hoenle UV Meter with its sensors
Hoenle UV Meter with its sensors. Image: Hoenle AG
Tacky coating, or wet beside the parts? Two causes on a UV line

Tacky coating, or wet beside the parts? Two causes on a UV line

Hoenle tested PT 4600 on boards in its lab (2024): broadband lamp, 200 W/cm, 60 mm, 100 µm film. Only the belt speed changed (3 and 4 m/min doses scaled from the 2 m/min measurement).

Belt speed
UVA dose
2,236 mJ/cm²
Surface
tacky
Colour
blue

Slight tack right after UV is normal for PT 4600: moisture finishes the cure in 2–3 days. ELANTAS confirmed 3 m/min is fine. Judge by dose and tack, not by colour: the change from blue to green/yellow also depends on lamp, film thickness and humidity.

Work out your own line: PT 4600 under an LED Powerline ACIC 820 XP

The same symptoms can have other causes too: lamp distance and angle, lamp wear, the spectrum, film thickness. All possible causes

Sources: Hoenle AG lab test on PT 4600 (2024); ELANTAS TDS for PT 4600, PT 4700 N, PL 5621 D. The beam colour is a convention; UV is invisible.

Bectron® coatings that cure under UV

Tab. 1Thin film · 1
CodeChemical baseViscosityOperating temperature
PL 5621D Epoxy400 ± 250 mPa·s (DIN 53019)-40 to +130 °C (short-term 160 °C)
Tab. 2Thick film · 4
CodeChemical baseViscosityOperating temperature
PT 4600 Polyurethane, one-component, solvent-free400–900 mPa·s (23 °C, DIN 53229)-40 to +125 °C
PT 4601 Polyurethane, one-component, solvent-free, thixotropic–-40 to +120 °C
PT 4606 Polyurethane (1-component, solvent-free)38,000 ± 8,000 mPa·s (DIN 53019, D = 10 s⁻¹, 23 °C)-40 to +120 °C
PT 4700 N Polyurethane (UV + moisture shadow-cure)200 ± 100 mPa·s (DIN 53019, 23 °C)–

Thin film · 1

Manufactured by ELANTAS Europe; ELANTAS Europe’s plants are certified to IATF 16949:2016 (ELANTAS presentation, 07/2024).

Hoenle AG LED UV curing systems

Hoenle AG builds LED curing systems, UV at 365–405 nm, from a hand pen to a conveyor line. A pen or a spot head cures single points. A hand-held or area unit cures a field, for example 137 × 75 mm (UVAHAND LED) or 200 × 50 mm (LED Spot 200 HP IC). A line unit cures a strip across the belt, and a chamber or a table-top conveyor cures whole parts and small boards.

Render: compact Hoenle AG LED heads irradiate a small optical part from four sides
Render: compact Hoenle AG LED heads for the bluepoint LED eco irradiate a small optical part from four sides (active alignment). Image: Hoenle AG

What we do on a UV line

We calculate which unit reaches the dose in your coating’s datasheet at your belt speed. For an LED line we confirm the cure in a trial on your own part. Hoenle AG standard units, accessories and spare parts: about 4–5 weeks from order. Custom systems: lead time per quote.

Next to this: Conformal coating · Printed electronics

Ask for a sample, a TDS, a quote or a dose calculation

Tell us what you need. We reply within 24 hours, in Romanian or English.

What do you need?

The button opens your email program with the inquiry filled in; you send it from there. We use these details only to answer this inquiry. Privacy notice

Contact directly

Alexandru Nichifor
Sales & technical support

+40 771 709 622

nichiforlx@nalteksolutions.com

Naltek Solutions S.R.L.