Why a UV-cured conformal coating stays tacky

18 October 2026 · Checked against the ELANTAS Bectron PT 4600 TDS N°1875 Rev. 2 (02/2024, pp. 2–3) and the PT 4601 TDS dated 07/02/2012 (pp. 2–3, newest on file) on 2026-11-12

Render: transparent conformal coating over SMD components on a dark PCB
Render: transparent conformal coating over SMD components on a dark PCB. Image: Hoenle AG

A UV-cured conformal coating that stays tacky has usually received too little UVA dose, or the tacky area lies in a shadow where the coating cures by moisture instead of light. For Bectron® PT 4600, the ELANTAS TDS (02/2024) specifies 2,500–3,500 mJ/cm² UVA (about 5 s at 3,000 mJ/cm² for a 200 ± 50 µm film), and 2 to 3 days for shadow areas.

Short answer: match the symptom to the TDS

SymptomLikely causeWhat the PT 4600 TDS says (TDS 02/2024, p. 2)
Open areas tacky or soft right after the UV tunnelUVA dose below the TDS value, or a film outside the thickness the dose refers to3000 mJ/cm² for a usual film thickness of 200 ± 50 µm, curing in approx. 5 s
Hard on open areas, soft under componentsShadow area, still curing by moisture“Post-curing by moisture in shadow areas takes 2 to 3 days.”
Cured, but properties below expectationPre-curing by daylight or UV inspection lamps before the tunnel“Sunlight or UV inspection lamps will start pre-curing, preventing the full development of the properties of the coating.”
Bubbles in the filmResidual washing water on the board“Residual water from washing the PCB can cause bubbles.”

What the coating needs: 2,500–3,500 mJ/cm² UVA

PT 4600 is a solvent-free one-component polyurethane thick-film coating, cured by UV irradiation and/or by moisture (TDS 02/2024, p. 2). PT 4601 is its thixotropic version for selective areas. Both TDSs give the same dose window; they refer it to different film thicknesses.

PropertyPT 4600PT 4601UnitMethod / source
UVA dose, mJ/cm²2,500–3,5003000 ± 500mJ/cm²PT 4600: TDS 02/2024 p. 3; PT 4601: TDS 07/02/2012 Table 2
Exposure time at that dose, s3–75 ± 2sPT 4600: TDS 02/2024 p. 3; PT 4601: Table 2
Film thickness the dose refers to, µm200 ± 50300 ± 50µmTDS p. 2
UV cure time, s5–10, “depending of the used type and power of the UV-lamp”5–10sTDS p. 2
Conveyor speed, m/min1–2.51–2.5m/minTDS p. 2
Viscosity as supplied, mPa·s400–900 (DIN 53229)1700 ± 600 (DIN 53019, D = 20 s⁻¹)mPa·s23 °C; PT 4600: TDS 02/2024 p. 3; PT 4601: Table 1
Hardness, cured, Shore A60–7065 ± 5Shore AISO 868, 23 °C; PT 4600: TDS 02/2024 p. 3; PT 4601: Table 4
Temperature range, cured, °C−40 to +125−40 to +120°CPT 4600: TDS 02/2024 p. 2–3; PT 4601: Table 3

Both TDSs say “UVA” and give no wavelength. We confirm with ELANTAS, case by case, whether a 365, 385, 395 or 405 nm LED head suits PT 4600 before we match a Hoenle unit to it. The 02/2024 revision gives the same dose window as the 2012 editions, written as 2,500–3,500 mJ/cm² instead of 3000 ± 500.

Reading the colour indicator: blue to green/yellow

PT 4600 is a “transparent thick film coating” (TDS 02/2024, p. 2) that is blue before cure; PT 4601 is blue as supplied (TDS 07/02/2012, Table 1). Both TDSs state that “a colour change from blue to green/yellow indicates the degree of UV-curing” (PT 4600: TDS 02/2024, p. 2). Open areas that are still blue after the tunnel show a low degree of UV cure by that indicator. The TDSs give no colour-versus-dose scale, so the colour confirms that UV reached an area; it does not replace a dose figure.

Shadow areas under components: 2–3 days, full properties after 2 weeks

Light does not reach the coating under tall components, connectors and BGAs. PT 4600 cures there by moisture: “Post-curing by moisture in shadow areas takes 2 to 3 days. Full polymerisation of the last <5 % will take place over 2 weeks achieving full properties of the material” (TDS 02/2024, p. 2; same wording in the PT 4601 TDS).

Time after the UV tunnelState of shadow areas per the PT 4600 TDS
0 to 2–3 daysMoisture post-cure in progress; soft coating under components is within what the TDS describes
2–3 daysMoisture post-cure complete
Up to 2 weeksLast <5 % polymerises; full material properties reached

A tack test on shadow areas straight after the tunnel therefore measures an intermediate state, not the final one.

Pre-curing before the lamp: daylight and UV inspection lamps

The PT 4600 TDS states: “The UV reactivity is high, so sunlight or UV inspection lamps will start pre-curing, preventing the full development of the properties of the coating” (TDS 02/2024, p. 2). The PT 4601 TDS carries the same warning. Coated boards that wait near windows, or that are checked for wet coverage under a UV inspection lamp before the tunnel, are exposed to this.

Conveyor speed and heat: the 1–2.5 m/min window

The TDS sets the belt speed: “The conveyor speed should be 1-2.5 m/min to limit influence of heat” (PT 4600 TDS 02/2024, p. 2). Slowing the belt below 1 m/min raises the dose but leaves that window. Inside the window, dose rises only with higher irradiance at the board, a shorter working distance or an additional lamp; doses from consecutive lamps add. The arithmetic is in the guide on UV dose on a conveyor, and the UV dose calculator runs it for your lamp.

Storage and moisture: why an opened container matters

PT 4600 cures by moisture as well as by UV (TDS 02/2024, p. 2). For that reason the TDS asks for sealed containers, “as the product is moisture sensitive”, and allows complete dipping or selective flooding only “in a machine with controlled atmosphere to exclude moisture”.

Storage itemPT 4600PT 4601Source
Shelf life in closed original containers6 months: cartridges and 5 kg bladder bag at 5–10 °C; 5 kg steel pail at −10 to 25 °C3 months at max. 5 °CPT 4600: TDS 02/2024 p. 2–3; PT 4601: TDS 07/02/2012
Recommended maximum storage temperatureNot stated in the 02/2024 TDS (storage by pack, see above)5 °CPT 4601: TDS 07/02/2012
Longer storageNot stated in the 02/2024 TDS−18 °CPT 4601: TDS 07/02/2012
ContainersSealed; product is moisture sensitiveSealed; product is moisture sensitiveTDS p. 2

What to check on your line

CheckTarget from the TDSWhy
UVA dose at the board2,500–3,500 mJ/cm²The dose the TDS cure data refers to (TDS 02/2024, p. 3)
Film thickness200 ± 50 µm (PT 4600); 300 ± 50 µm (PT 4601)The thickness each TDS ties to that dose (p. 2)
Belt speed1–2.5 m/minTDS limit for heat (p. 2)
Colour of open areas after the tunnelGreen/yellow, no longer blueTDS cure indicator (p. 2)
Light exposure before the tunnelNo sunlight, no UV inspection lampTDS caution on pre-curing (p. 2)
Container handlingSealed, stored per the table aboveMoisture sensitivity (p. 2)
Batch viscosity400–900 mPa·s (PT 4600, DIN 53229, 23 °C)Sales specification (TDS 02/2024, p. 3)
Board conditionClean, dry, free from grease; low-solids flux or alcohol-based cleanersTDS preparation section (p. 2)
Time before judging shadow areas2–3 days; full properties after 2 weeksTDS curing section (p. 2)

Getting a dose calculation for your line

Dose is irradiance multiplied by exposure time. Naltek calculates it for your line from lamp type, lens, working distance and belt speed, and compares the result with the 2,500–3,500 mJ/cm² in the PT 4600 TDS. If you want a measured value as well, we measure it on site during a visit.

Through the inquiry form, send the coating code, film thickness, belt speed, lamp model and lens, and working distance, and ask for the PT 4600 or PT 4601 TDS or a dose calculation.

Questions engineers ask

How long does PT 4600 take to cure under components?

Post-curing by moisture in shadow areas takes 2 to 3 days, and full polymerisation of the last <5 % takes place over 2 weeks, according to the ELANTAS PT 4600 TDS (02/2024, p. 2).

What UV dose does PT 4600 need?

2,500–3,500 mJ/cm² UVA in 3–7 s; for a usual film thickness of 200 ± 50 µm and 3,000 mJ/cm², curing takes about 5 s (PT 4600 TDS 02/2024, p. 2–3). The PT 4601 TDS (07/02/2012) gives 3000 ± 500 mJ/cm² for 300 ± 50 µm.

Why does the coating change colour from blue to green?

The PT 4600 and PT 4601 TDSs state that a colour change from blue to green/yellow indicates the degree of UV curing. The TDSs give no colour-versus-dose scale, so the colour is a visual check, not a dose measurement.

Can I inspect boards under a UV lamp before curing?

Not with PT 4600 or PT 4601. Both TDSs warn that the UV reactivity is high, so sunlight or UV inspection lamps start pre-curing and prevent the full development of the coating's properties.

Why not just run the conveyor slower to add dose?

The PT 4600 TDS says the conveyor speed should be 1–2.5 m/min to limit the influence of heat. To add dose inside that window, the irradiance at the board has to rise, or a second lamp has to be added.

Application pages: Conformal coating · UV curing

Sources: ELANTAS Bectron PT 4600 technical data sheet N°1875 Rev. 2, 02/2024, p. 2 (curing, caution, storage) and p. 3 (specifications and properties); ELANTAS Bectron PT 4601 technical data sheet, 07/02/2012, pp. 2–3 (newest on file).

Products in this guide

Request TDS or a sample

Ask for a sample, a TDS, a quote or a dose calculation

Tell us what you need. We reply within 24 hours, in Romanian or English.

What do you need?

The button opens your email program with the inquiry filled in; you send it from there. We use these details only to answer this inquiry. Privacy notice

Contact directly

Alexandru Nichifor
Sales & technical support

+40 771 709 622

nichiforlx@nalteksolutions.com

Naltek Solutions S.R.L.
Sat Comori, Com. Gurghiu, nr. 81, jud. Mureș 547298